摘要
A new method on the fabricating techniques of the BaAl2S4:Eu sputtering target is introduced, which is called powder sintering method. The particular fabricating conditions based on the BaAl2S4: Eu sample are illustrated as comminution, rubbing, sintering and hot-pressing. The photoluminescence spectrum of the BaAl2S4:Eu films shows that there are 470nm PL emission peaks of the as-fabricated phosphor films excited by 300nm ultraviolet radiations. The BaAl2S4 :Eu films contain more oxygen than other elements such as Ba,Al,S,Eu, and the content of Al aggrandizes when the sputtering power increases and the content of S decreases when the pressure increases in the vacuum chamber.
源语言 | 英语 |
---|---|
页(从-至) | 785-787 |
页数 | 3 |
期刊 | Guangxue Jishu/Optical Technique |
卷 | 35 |
期 | 5 |
出版状态 | 已出版 - 9月 2009 |