Abstract
In order to further improve the oxidation protective ability of (ZrB2-SiC)/SiC coated graphite, ferrocene was introduced into the outer ZrB2-SiC coatings during pack cementation process. The ferrocene addition increased the porosity of the outer ZrB2-SiC coatings, which was favorable to thermal shock resistance of (ZrB2-SiC)/SiC coated specimens. The ZrB2-SiC coating with 3 wt% ferrocene (ZS50-3f) has optimum oxidation protective ability. Its weight retention after 15 thermal shock cycles between 1500 °C and room temperature was 96. 2%. The weight loss of ZS50-3f was only 0.2% after 19 h oxidation at 1500 °C.
| Original language | English |
|---|---|
| Pages (from-to) | 2654-2661 |
| Number of pages | 8 |
| Journal | Ceramics International |
| Volume | 42 |
| Issue number | 2 |
| DOIs | |
| Publication status | Published - 1 Feb 2016 |
| Externally published | Yes |
Keywords
- C. Thermal Shock Resistance
- Coating
- Ferrocene
- Oxidation resistance
- ZrB-SiC